Author: R. Sejnoha
Publisher: Philadelphia : American Society for Testing and Materials
ISBN:
Category :
Languages : en
Pages : 24
Book Description
Iodine-induced Stress Corrosion Cracking of Fixed Deflection Stressed Slotted Rings of Zircaloy Fuel Cladding
Author: R. Sejnoha
Publisher: Philadelphia : American Society for Testing and Materials
ISBN:
Category :
Languages : en
Pages : 24
Book Description
Publisher: Philadelphia : American Society for Testing and Materials
ISBN:
Category :
Languages : en
Pages : 24
Book Description
Zirconium in the Nuclear Industry
Author:
Publisher: ASTM International
ISBN:
Category :
Languages : en
Pages : 627
Book Description
Publisher: ASTM International
ISBN:
Category :
Languages : en
Pages : 627
Book Description
Zirconium in the Nuclear Industry
Author: J. H. Schemel
Publisher: ASTM International
ISBN: 9780803106017
Category : Business & Economics
Languages : en
Pages : 656
Book Description
Publisher: ASTM International
ISBN: 9780803106017
Category : Business & Economics
Languages : en
Pages : 656
Book Description
Iodine Induced Stress Corrosion Cracking of Zircaloy Fuel Cladding Materials
Author:
Publisher:
ISBN:
Category : Stress corrosion
Languages : en
Pages : 165
Book Description
Publisher:
ISBN:
Category : Stress corrosion
Languages : en
Pages : 165
Book Description
Fracture of Zircaloy-2 in an Environment Containing Iodine
Author: B. van der Schaaf
Publisher:
ISBN:
Category : Biaxial stresses
Languages : en
Pages : 16
Book Description
Many Zircaloy cladding failures and the results of out-of-pile iodine stress corrosion tests are so similar as to suggest that fission of uranium produces enough iodine to attack the cladding locally. This paper presents a study of the effects of iodine on the fracture of Zircaloy-2 sheet being stressed very locally. Discs produced from Zircaloy-2 sheet were bent biaxially by pressing an indentor into the center of the disc. The force necessary to penetrate the discs decreased when either the initial amount of iodine or the temperature was increased, for cold-worked as well as recrystallized Zircaloy-2. Uniaxial short-time creep tests and tests with stressed slotted rings, both performed in environments containing iodine, did not result in stress corrosion cracking.
Publisher:
ISBN:
Category : Biaxial stresses
Languages : en
Pages : 16
Book Description
Many Zircaloy cladding failures and the results of out-of-pile iodine stress corrosion tests are so similar as to suggest that fission of uranium produces enough iodine to attack the cladding locally. This paper presents a study of the effects of iodine on the fracture of Zircaloy-2 sheet being stressed very locally. Discs produced from Zircaloy-2 sheet were bent biaxially by pressing an indentor into the center of the disc. The force necessary to penetrate the discs decreased when either the initial amount of iodine or the temperature was increased, for cold-worked as well as recrystallized Zircaloy-2. Uniaxial short-time creep tests and tests with stressed slotted rings, both performed in environments containing iodine, did not result in stress corrosion cracking.
4th International Conference on CANDU Fuel
Author:
Publisher:
ISBN:
Category : Nuclear fuels
Languages : en
Pages : 516
Book Description
Publisher:
ISBN:
Category : Nuclear fuels
Languages : en
Pages : 516
Book Description
Pellet-cladding Interaction Failures in Water Reactor Fuel Rods
Author: Bernardo N. Nobrega
Publisher:
ISBN:
Category : Nuclear fuel claddings
Languages : en
Pages : 270
Book Description
Publisher:
ISBN:
Category : Nuclear fuel claddings
Languages : en
Pages : 270
Book Description
Iodine-Induced Stress Corrosion of Zircaloy Fuel Cladding
Author: L. Brunisholz
Publisher:
ISBN:
Category : Crack propagation
Languages : en
Pages : 17
Book Description
Because of its impact on nuclear power plant reliability, fuel cladding failure induced by pellet cladding interaction is a problem of major concern. It is usually analyzed as stress corrosion cracking caused by volatile fission products like iodine.
Publisher:
ISBN:
Category : Crack propagation
Languages : en
Pages : 17
Book Description
Because of its impact on nuclear power plant reliability, fuel cladding failure induced by pellet cladding interaction is a problem of major concern. It is usually analyzed as stress corrosion cracking caused by volatile fission products like iodine.
Initial Report on Stress-corrosion-cracking Experiments Using Zircaloy-4 Spent Fuel Cladding C-rings
Author: H. D. Smith
Publisher:
ISBN:
Category : Corrosion and anti-corrosives
Languages : en
Pages : 70
Book Description
Publisher:
ISBN:
Category : Corrosion and anti-corrosives
Languages : en
Pages : 70
Book Description
INIS Atomindex
Author:
Publisher:
ISBN:
Category : Nuclear energy
Languages : en
Pages : 1250
Book Description
Publisher:
ISBN:
Category : Nuclear energy
Languages : en
Pages : 1250
Book Description